4.0 Welding Hints
Because of the multitude of and great differences in the important points for welding only the very basic operations
for the most common electrodes for low-carbon steels, the rutile- or rutile/cellulose type electrode, are introduced here.
In the case that other electrodes have to be used, the electrode manufacturers supply upon request all relevant
information for the type of special electrode to be used.
Always make some trial welds on scrap material. Select electrode diameter and welding current as per Table 1 (shown
on page 5). Attach earth clamp to work piece and place electrode into electrode holder as described earlier. Now hold
the electrode tip approx. 2 cm / 1 inch above the starting point of your welding seam. Hold the welding shield in front
of your face and draw the electrode with a short stroke along the groove. Through the welding shield you watch the
arc, keeping it to a length of 1 to 1.5 times the electrode diameter.
Remove slag only after it has cooled down and is no longer glowing.
If an interrupted weld is to be continued, the slag at the end of the already finished weld must be removed. Then the
arc can be started either in the groove or on the weld, as described earlier, and then moved to the end of the weld,
which has to be thoroughly melted for good fusion. Welding is then continued normally.
The welder has to keep the arc at the same length, that is the electrode burn-off is compensated by feeding the
electrode into the weld. At the same time the welder has to watch the weld pool for even penetration and width.
Welding is always done from left to right (backhand welding).
At the end of the welding seam the electrode can not simply be lifted or pulled from the weld, this creates porous end
craters, which weaken the weld. To correctly terminate a weld the electrode is held for a short moment at the end of
the weld seam, then lifted in an arc over the just laid weld.
The correct arc length is important for a good weld, because with too short or too long an arc both welding current and
working voltage change. A low working voltage causes insufficient penetration. Too high or too low welding current
gives a poor welding seam. Too long an arc does not sufficiently melt the parent material, resulting in high spatter
losses. Also the air, with its detrimental substances like hydrogen and nitrogen, may get access to the weld pool.
For a good weld the work angle of the electrode (or electrode inclination angle) is of substantial importance. The
inclination should be 70° - 80° to the welding direction. With the work angle too steep slag will run under the weld pool,
too flat an work angle causes the arc to spatter, in both cases the result is a porous, weak welding seam (see pictures
5 - 7).
wrong
arc too long
(Pic. 3)
correct
approx. 1 - 1.5 the electrode-Ø
(Pic. 4)
< 70°
welding direction
(Pic. 6)
(Pic. 5)
> 80°
welding direction
(Pic. 7)
70-80°
welding direction
wrong
wrong correct
wrong
(Pic. 8)
correct
(Pic. 9)
17

Brauchen Sie Hilfe? Stellen Sie Ihre Frage.

Forenregeln
1

Forum

elektra-beckum-sk200

Suche zurücksetzen

  • habe ein beckum schweisgerät 220v 380v stecker 380v fehlt da sind crei kabel gelb grün blau und braun we wird der stecker da angeschlosen da steht auf dem gelben zettel siehe betriebsanleitung seite 5 die ich leider nicht habe Eingereicht am 3-6-2023 11:35

    Antworten Frage melden

Missbrauch melden von Frage und/oder Antwort

Libble nimmt den Missbrauch seiner Dienste sehr ernst. Wir setzen uns dafür ein, derartige Missbrauchsfälle gemäß den Gesetzen Ihres Heimatlandes zu behandeln. Wenn Sie eine Meldung übermitteln, überprüfen wir Ihre Informationen und ergreifen entsprechende Maßnahmen. Wir melden uns nur dann wieder bei Ihnen, wenn wir weitere Einzelheiten wissen müssen oder weitere Informationen für Sie haben.

Art des Missbrauchs:

Zum Beispiel antisemitische Inhalte, rassistische Inhalte oder Material, das zu einer Gewalttat führen könnte.

Beispielsweise eine Kreditkartennummer, persönliche Identifikationsnummer oder unveröffentlichte Privatadresse. Beachten Sie, dass E-Mail-Adressen und der vollständige Name nicht als private Informationen angesehen werden.

Forenregeln

Um zu sinnvolle Fragen zu kommen halten Sie sich bitte an folgende Spielregeln:

Neu registrieren

Registrieren auf E - Mails für Elektra Beckum SK200 wenn:


Sie erhalten eine E-Mail, um sich für eine oder beide Optionen anzumelden.


Das Handbuch wird per E-Mail gesendet. Überprüfen Sie ihre E-Mail.

Wenn Sie innerhalb von 15 Minuten keine E-Mail mit dem Handbuch erhalten haben, kann es sein, dass Sie eine falsche E-Mail-Adresse eingegeben haben oder dass Ihr ISP eine maximale Größe eingestellt hat, um E-Mails zu erhalten, die kleiner als die Größe des Handbuchs sind.

Ihre Frage wurde zu diesem Forum hinzugefügt

Möchten Sie eine E-Mail erhalten, wenn neue Antworten und Fragen veröffentlicht werden? Geben Sie bitte Ihre Email-Adresse ein.



Info